A-A-1447A
Test Method A- Test for wet tensile strength according to TAPPI T 456, except that samples of towels shall first be placed in a 105oC oven for 4 minutes.
Test Method B- Test in accordance with TAPPI T 432 using 0.1 ml of white mineral oil, 80-90 S.U. (Saybolt Universal) viscosity, +30 Saybolt color, N.F. grade in lieu of water.
Test Method C- Condition the specimen in accordance with TAPPI T 402. Weigh each specimen of size 4x4 (+ 1/8) inches, and immerse them in distilled water at 25oC for 3 minutes (+ 10 seconds). Remove the specimens by lifting them at one corner until their surfaces are vertical to the floor, and allow the excess water to drain off for 60 + 10 seconds. Place each in a tared weighing bottle and reweigh. Calculate the percent absorption to the nearest one percent as follows:
Percent absorption =
Wet weight- Dry weight
X100
Dry weight
Test Method D- Follow the procedures in Test Method C using oil as specified in Test Method B in lieu of water. Drain time for immersed sample should be 20 + 2 minutes.
Workmanship. The towels shall be soft, pliable, smooth, and clean. Towels shall not contain holes, tears, cuts, wrinkles, dirt, and foreign material which will adversely affect the appearance or serviceability of the towels.
Regulatory requirements. The offeror/contractor is encouraged to use recovered materials in accordance with Public Law 94-580 to the maximum extent practicable.
Preservation, packaging, packing, labeling and marking. Preservation, packaging, packing, labeling, and marking shall be as specified in the contract or order.
Notes: TAPPI test methods are available from the Technical Association of the Pulp and Paper Industry, Technology Park/Atlanta, P.O. Box 105113, Atlanta, GA 30348.
DoD has waived coordination of this document.
PREPARING ACTIVITY: GSA-FSS |
For Parts Inquires submit RFQ to Parts Hangar, Inc.
© Copyright 2015 Integrated Publishing, Inc.
A Service Disabled Veteran Owned Small Business